crown
Problem:
Disturbed
joint.
Characteristics:
Rough
appearance
with
questionable
adhesion.
Cause:
Fig.
7.7
Disturbed
Joint
Movement
of
wire/joint
during
cool-off
stage.
Remedy:
Use
of
holding
vice
or
similar
tool
to
help
prevent
movement.
Problem:
Cold
solder
joint.
Characteristics:
Joint
with
dull,
frosty
appearance;
often
has
poor
adhesion
as
well
as
imperfect
shaping.
Cause:
Fig.
7.8
Cold
Solder
Joint
Too
much
heat
applied
(flux
is
boiled
off
before
Remedy:
oxide
removal
action
takes
place).
Correct
matching
of
iron/tip
to
specific
job.
Correct
solder
flux
combination
is
also
important.