Troubleshooting
3A1320L 39
Applying Material
Problem Cause Solution
Ragged line edges when extruding Dirty screed box CAREFULLY clean box. Discharge
opening and screed box plate run-
ners need to be free of debris.
Cold material temperatures Heat material as required.
Marking speed too fast Slow ThermoLazer speed.
Rough material surface when extrud-
ing
Overheated material Reduce heat.
Moisture on road surface Allow road surface moisture to dry.
Rough road surface Smooth road surface.
Screed box low on material Add material to screed box.
EXAMPLES:
Correct line application will produce a full straight line with sharp edges; correct color,
thickness and width; a firm bond to the surface; and have uniform reflectivity.
Insufficient adhesion (material bulges
at beginning of line)
Material temperature too low
ThermoLazer speed too fast
Debris on road
Surface temperature too cold
Raise material temperature.
Decrease speed of
ThermoLazer.
Clear debris from road.
Wait for temperature of surface
to raise.
Rough and bumpy line Debris on surface
Crust from overheated material
Debris caught in screed box
Material not covering road high
spot
Clear debris from surface.
Lower material temperature.
Clean debris from screed box.
Adjust screed box line thickness.
Gas bubbles in line Moisture or solvent on surface
Material is overheated
Remove solvent from surface.
Lower temperature of material.
Ragged edges and gaps in line Material temperature is too low
ThermoLazer speed is too fast
Raise material temperature.
Wait for change in ambient condi-
tions to remove moisture.
Reduce ThermoLazer speed.