TABLE I
Glass Electrical And Thermal Properties
Log
10
Loss Volume Dielectric Softening
Glass Factor Resistivity Constant Temp. °C Description
7940 .0038 11.8 3.8 1580 Quartz (fused silica)
1724 .0066 13.8 6.6 926 Aluminosilicate
7070 .25 11.2 4.1 ---- Low loss borosilicate
8161 .50 12.0 8.3 604 High lead
Sylgard .58 13.0 2.9 ---- #184 Coating cmpd.
7059 .584 13.1 5.8 844 Barium-borosilicate
7760 .79 9.4 4.5 780 Borosilicate
EG-6 .80 9.6 7.0 625 High lead
0120 .80 10.1 6.7 630 High lead
EG-16 .90 11.3 9.6 580 High lead
7040 1.00 9.6 4.8 700 Kovar seal borosilicate
KG-12 1.00 9.9 6.7 632 High lead
1723 1.00 13.5 6.3 910 Aluminosilicate
0010 1.07 8.9 6.7 625 High lead
7052 1.30 9.2 4.9 710 Kovar seal borosilicate
EN-1 1.30 9.0 5.1 716 Kovar seal borosilicate
7720 1.30 8.8 4.7 755 Tungsten seal borosilicate
7056 1.50 10.2 5.7 720 Kovar seal borosilicate
3320 1.50 8.6 4.9 780 Tungsten seal borosilicate
7050 1.60 8.8 4.9 705 Series seal borosilicate
KG-33 2.20 7.9 4.6 827 Kimax borosilicate
7740 2.60 8.1 5.1 820 Pyrex borosilicate
1720 2.70 11.4 7.2 915 Aluminosilicate
N-51A 3.70 7.2 5.9 785 Borosilicate
R-6 5.10 6.6 7.3 700 Soda lime
0080 6.50 6.4 7.2 695 Soda lime