78
9.2 Firing table for Finesse metal ceramic (Dentsply De Trey-Mode)
(Use honeycomb firing material carrier.)
Prog. Program Preheat/ Drying Preheat Vacuum Rate of Firing/ Vacuum- Firing
# Description Low Temp. Time Level Temp. Rise High Temp. Time Time
°C min min hPa °C/min °C min min
311 D-FIN-Pulver- 450 03:00 03:00 50 90 800 00:30 01:00
Opaker
312 D-FIN-Pasten- 450 05:00 03:00 50 90 790 00:06 00:30
Opaker
313 D-FIN-Joint Opaque/ 675 03:00 07:00 50 35 770 00:06 00:30
Margin/margin mod.
314 D-FIN-Korrektur- 450 05:00 03:00 50 90 760 00:06 00:30
Opaker
315 D-FIN-1
st
Main Firing 450 05:00 05:00 50 35 760 00:06 00:30
Opaque dentine,
Dentin,
Dentine effect
enamel,
gums
316 D-FIN-2
nd
Main Firing 450 05:00 05:00 50 35 750 00:06 00:30
Opaque dentine,
Dentin,
Dentine effect
enamel,
gums
317 D-FIN-Correction- 450 05:00 05:00 50 55 730 00:06 00:30
Firing
318 D-FIN-Glaze firing/ 450 03:00 03:00 – 70 750 – 00:06
Stains*
319 D-FAC-repair 450 05:00 05:00 50 35 810 00:06 00:30
porcelain
320 D-FAC-Shade 450 03:00 01:00 – 100 730 – 01:00
stain porcelain
D = Dentsply-Modus
FIN =
Finesse Metal ceramic
FAC = Finesse All Ceramic
* depending on desired degree of glaze
1
Caution!
Firing parameters not listed in the firing table must be set to “0” when entering values.
Caution! Do not use pressing socket for firing.
Notes: Make a test firing if required, and adjust firing temperatures or times. For a large number of objects, temperatures or times must
be increased appropriately.