Maintenance Manual LS8
Issued: December 2009
Copyright DG Flugzeugbau GmbH - any copy or publishing prohibited
Manual valid with the up-to-date cover page only
10-2
Foam
:
PVC foam Divinycell H 60, 8 mm thick, mass 60 kg/m²,
<wing shells>, <vertical tail fin> Manufacturer: Diab
PVC foam Divinycell H 80, 6 mm thick, mass 80 kg/m²,
<horizontal tail shells> Manufacturer: Diab
PVC foam Divinycell HP 80, 10 mm thick, mass 80 kg/m²,
<spar shearweb > Manufacturer: Diab
alternative
PVC foam Divinycell HT 70, 6/8/10 mm thick, mass 70 kg/m²,
<spar shearweb, horizontal tail>, Manufacturer: Diab
alternative
PVC foam Klegecell TR 75, 8mm thick, mass 75 kg/m²,:
<wing shells> Manufacturer Polimex S.p.A.
Foam Rohacell 71, 2.5 mm thick, mass 70 kg/m²,
<control surfaces> Manufacturer: Röhm
Only LS8-a, LS8-b, LS8-18
Corrugated paper E-Wellpappe, einseitig (370) API 80 (80g/m²)
<Aileron> Manufacturer:Ludwig Clemens
Glue for Plexiglas
To attach the canopy:
glue Teroson Macroplast UK 8303B60
hardener Teroson Macroplast UK5400
mixing ratio: 6 : 1 by mass
thickened with Aerosil.
To repair cracks in the canopy:
Röhm Acrifix 192 which hardens by exposure to light.
Filler
For gluing, the resin-hardener mix should be thickened with chopped cotton
fibres FL l f. (add enough so that the resin no longer flows). The surfaces to be
glued should be wetted with non-thickened resin + hardener before.
To glue foam pieces into place when repairing sandwich sections and to fill in
irregularities and gaps etc. around the repair, Microballoon BJO - 0930 can be
used mixed with the resin + hardener. Application and mixing is the same as for