GENERAL INFORMATION
90-857046R1 NOVEMBER 2001 Page 1C-21
Painting Procedures
Cleaning & Painting Aluminum Propellers & Gear Housings
WARNING
Avoid serious injury from flying debris. Avoid serious injury from airborne par-
ticles. Use eye and breathing protection with proper ventilation.
PROPELLERS
1. Sand the entire area to be painted with 3M 120 Regalite Polycut or coarse Scotch-Brite,
disc or belts.
2. Feather edges of all broken paint edges. Try not to sand through the primer.
3. Clean the surface to be painted using PPG Industries DX330 Wax and Grease Remover
or equivalent (Xylene or M.E.K.).
4. If bare metal has been exposed, use Mercury/Quicksilver Light Gray Primer.
5. Allow a minimum of 1 hour dry time and no more than 1 week before applying the finish coat.
6. Apply the finish coat using Mercury/Quicksilver EDP Propeller Black.
GEAR HOUSINGS
The following procedures should be used in refinishing gear housings. This procedure will
provide the most durable paint system available in the field. The materials recommended
are of high quality and approximate marine requirements. The following procedure will pro-
vide a repaint job that compares with a properly applied factory paint finish. It is recom-
mended that the listed materials be purchased from a local Ditzler Automotive Finish Supply
Outlet. The minimum package quantity of each material shown following is sufficient to refin-
ish several gear housings.
Procedure:
1. Wash gear housing with a muriatic acid base cleaner to remove any type of marine
growth, and rinse with water, if necessary.
2. Wash gear housing with soap and water, then rinse.
3. Sand blistered area with 3M 180 grit sandpaper or P180 Gold Film Disc to remove paint
blisters only. Feather edge all broken paint edges.
4. Clean gear housing thoroughly with (DX-330) wax and grease remover.
5. Spot repair surfaces where bare metal is exposed with (DX-503) alodine treatment.
IMPORTANT: Do not use any type of aerosol spray paints as the paint will not properly
adhere to the surface nor will the coating be sufficiently thick to resist future paint
blistering.
6. Mix epoxy chromate primer (DP-40) with equal part catalyst (DP-401) per manufacturers
instructions, allowing proper induction period for permeation of the epoxy primer and catalyst.
7. Allow a minimum of one hour drying time and no more than one week before top coating
assemblies.
8. Use Ditzler Urethane DU9000 for Mercury Black, DU34334 for Mariner Grey, and
DU35466 for Force Charcoal, and DU33414M for Sea Ray White. Catalyze all four col-
ors with Ditzler DU5 catalyst mixed 1:1 ratio. Reduce with solvents per Ditzler label.

Table of Contents

Questions and Answers:

Question and Answer IconNeed help?

Do you have a question about the Mercury 40 FourStroke and is the answer not in the manual?

Mercury 40 FourStroke Specifications

General IconGeneral
BrandMercury
Model40 FourStroke
CategoryOutboard Motor
LanguageEnglish

Related product manuals